Catalytic converters that are designed to remove toxic gases and pollutants from car exhaust gases contain the precious metals Pt, Pd and Rh. When the car reaches the end of life the converter is scrapped and the precious metals are recovered in a recycling chain comprising several different stakeholders, from scrap yards to toll refineries. Due to their high value, accurate analysis of the precious metal content is critical to ensure every stakeholder receives a fair share for their contribution. This application note shows a safe, easy and accurate method for providing data everyone will trust.
Catalytic converters that are designed to remove toxic gases and pollutants from car exhaust gases contain the precious metals Pt, Pd and Rh. When the car reaches the end of life the converter is scrapped and the precious metals are recovered in a recycling chain comprising several different stakeholders, from scrap yards to toll refineries. Due to their high value, accurate analysis of the precious metal content is critical to ensure every stakeholder receives a fair share for their contribution. This application note shows a safe, easy and accurate method for providing data everyone will trust.
Measurements were performed using a Malvern Panalytical Epsilon 1 EDXRF spectrometer, equipped with a 50 kV silver (Ag) anode X-ray tube, 6 software-selectable filters, a high resolution SDD10 silicon drift detector and a 1 position sample position.
Thirty-three car catalyst samples supplied by several customers were used to create the application. The precious metals were determined by fire assay or inductively coupled plasma spectroscopy. The majors in the matrix have been determined using Malvern Panalytical’s solutions WROXI and Omnian. The standards were analyzed in the form of loose powder in a P1 assembled sample cup with a 6 μm polypropylene foil. The setup samples were oven-dried. 8 grams of each powder was put in sample cups and slightly compressed using a steel cylinder, illustrated in Figure 1.
				
              ![[Figure 1 AN220330-fast-analysis-precious-metals-catalytic-converters.jpg] Figure 1 AN220330-fast-analysis-precious-metals-catalytic-converters.jpg](https://dam.malvernpanalytical.com/c331b39c-d91f-45e9-8e71-ae6800f2b236/Figure%201%20AN220330-fast-analysis-precious-metals-catalytic-converters_Original%20file.jpg) 
				
			
Figure 1. Loose powder sample representation. Loose powders very slightly compressed in the sample cup using a steel cylinder.
3 different measurement conditions were used to measure the 3 precious metals and major compounds in the samples. Measuring the total matrix improves the flexibility of the method and makes it applicable for different catalytic converter materials. The total measurement time was set to 5 minutes per sample. In this application note only the three precious metals are reported.
| Elements | kV | uA | Filter | Meas. time (s) | 
|---|---|---|---|---|
| Pt , Ni, Zn, Sr, Zr, W, Pb | 50 | 200 | Ag | 60 | 
| Rh, Pd, Ba | 50 | 200 | Cu - thick | 180 | 
| S, K, Ca, Ti, Mn, Fe, La, Ce, Nd | 14 | 714 | Al - thin | 60 | 
Table 1. Measurements conditions.
Figures 2, 3 and 4 show the resulting calibration graphs for Pt, Rh and Pd in catalytic monoliths. The graphs show very good correlation between the certified concentrations and the measured intensities. Detailed calibration results for the precious metals are listed in Table 2. The RMS (Root Mean Square) value is equivalent to 1 sigma standard deviation.
| Compounds | Concentration range | RMS (ppm)* | Correlation Coefficient | 
|---|---|---|---|
| Pt (ppm) | 0 –1992 | 52.5 | 0.9968 | 
| Rh (ppm) | 0 – 585 | 10.6 | 0.9959 | 
| Pd (ppm) | 0 – 8776 | 92.6 | 0.9991 | 
Table 2. Calibration details (* RMS: The more accurate calibrations have the smaller RMS values).
				
              ![[Figure 2 AN220330-fast-analysis-precious-metals-catalytic-converters.jpg] Figure 2 AN220330-fast-analysis-precious-metals-catalytic-converters.jpg](https://dam.malvernpanalytical.com/5f317a0d-b1c3-4a74-956d-ae6800f2b35a/Figure%202%20AN220330-fast-analysis-precious-metals-catalytic-converters_Original%20file.jpg) 
				
			
				Figure 2. Calibration graph for Pt in catalytic converters
				
			
				
              ![[Figure 3 AN220330-fast-analysis-precious-metals-catalytic-converters.jpg] Figure 3 AN220330-fast-analysis-precious-metals-catalytic-converters.jpg](https://dam.malvernpanalytical.com/6c2a6b6e-ea50-4149-a895-ae6800f2b309/Figure%203%20AN220330-fast-analysis-precious-metals-catalytic-converters_Original%20file.jpg) 
				
			
				Figure 3. Calibration graph for Rh in catalytic converters
				
			
				
              ![[Figure 4 AN220330-fast-analysis-precious-metals-catalytic-converters.jpg] Figure 4 AN220330-fast-analysis-precious-metals-catalytic-converters.jpg](https://dam.malvernpanalytical.com/8b26d7ba-1ed5-4b65-a671-ae6800f2b28a/Figure%204%20AN220330-fast-analysis-precious-metals-catalytic-converters_Original%20file.jpg) 
				
			
				Figure 4. Calibration graph for Pd in catalytic converters
				
			
The accuracy and instrument precision were tested by measuring multiple official certified reference materials (CRM’s) 20 times or 5 times consecutively. The certified and average measured concentrations, RMS and relative RMS values are presented in Table 3, demonstrating excellent accuracy and precision.
| Sample name (repeats) | Compounds | Certified conc. | Average conc. | RMS | Rel. RMS (%) | 
|---|---|---|---|---|---|
| NIST 2556 (20x) | Pt (ppm) | 697.4 +/- 6.3 | 695.6 | 7.2 | 1.1 | 
| Rh (ppm) | 51.2 +/- 0.5 | 53.9 | 2.0 | 3.7 | |
| Pd (ppm) | 326 +/- 1.6 | 322.8 | 7.2 | 2.2 | |
| NIST 2557 (20x) | Pt (ppm) | 1131 +/- 11 | 1189.6 | 13.2 | 1.1 | 
| Rh (ppm) | 135.1 +/- 1.9 | 141.6 | 2.2 | 1.6 | |
| Pd (ppm) | 233.2 +/- 1.9 | 236.9 | 3.6 | 1.5 | |
| ERM-EB504a (5x) | Pt (ppm) | 1414 +/- 9.0 | 1424.8 | 5.1 | 0.4 | 
| Rh (ppm) | 210 +/- 2.2 | 216.2 | 2.3 | 1.1 | |
| Pd (ppm) | 1596 +/- 11 | 1675.1 | 18.3 | 1.1 | |
| FLX 133 (5x) | Pt (ppm) | 465 +/- 32 | 462.1 | 4.0 | 0.9 | 
| Rh (ppm) | 242 +/- 4 | 237.6 | 4.0 | 1.7 | |
| Pd (ppm) | 1075 +/- 33 | 1093.8 | 15.3 | 1.4 | 
Table 3. Accuracy and precision testing on four commercially available certified reference materials.
The results clearly demonstrate the capability of Epsilon 1 for the analysis of metals Pt, Rh and Pd in catalytic converters. The repeatable sample positioning, outstanding sensitivity of the optical components combined with powerful software deconvolution algorithms allows the Epsilon 1 to provide accurate analysis for every measurement.
In 5 minutes, the Epsilon 1 will provide an accurate reading of the precious metal content you can trust. The shielding for the high energetic X-rays and safety locks in place guarantees every user safety while determining the value of their sample.