Collecting high-pressure Carbon Dioxide adsorption data on the AccuSorp HP: an analysis of molecular sieves and carbon materials

Carbon capture, utilization and storage (CCUS) remains a critical area of scientific research as the impacts of climate change are observed globally each year. A primary driver of global warming is the increasing concentration of carbon dioxide in the atmosphere, which has risen steadily since the onset of global industrialization, primarily resulting from the combustion of fossil fuels. Underscoring the urgency of this trend, the World Meteorological Organization reports that the past 11 years have comprised the warmest on record, with continued warming likely heading into the future (wmo.int). In response, research efforts have focused on developing advanced materials to mitigate emissions by capturing carbon dioxide both directly from ambient air as well as from emission point-sources. For these mitigation strategies to be fully realized, efficient capture must be accompanied by secure storage of carbon dioxide.

Multiple pathways exist for the subsequent storage and utilization of captured carbon dioxide. Sequestration strategies include injection into depleted oil and natural gas reservoirs, mineralization within deep geological rock formations, and utilization of carbon dioxide as a feedstock for the production of value-added products. Regardless of the targeted pathway, a comprehensive understanding of the porous materials engineered to store carbon dioxide under elevated pressures is critical.

In this study, the AccuSorp HP was utilized to evaluate high-pressure carbon dioxide adsorption isotherms across a diverse suite of materials, including molecular sieve 4A, 5A, 13X, and a commercial activated carbon from Supelco. This work establishes a framework for collecting high-pressure carbon dioxide adsorption data utilizing the advanced capabilities of the AccuSorp HP.

Introduction

Carbon capture, utilization and storage (CCUS) remains a critical area of scientific research as the impacts of climate change are observed globally each year. A primary driver of global warming is the increasing concentration of carbon dioxide in the atmosphere, which has risen steadily since the onset of global industrialization, primarily resulting from the combustion of fossil fuels. Underscoring the urgency of this trend, the World Meteorological Organization reports that the past 11 years have comprised the warmest on record, with continued warming likely heading into the future (wmo.int). In response, research efforts have focused on developing advanced materials to mitigate emissions by capturing carbon dioxide both directly from ambient air as well as from emission point-sources. For these mitigation strategies to be fully realized, efficient capture must be accompanied by secure storage of carbon dioxide.

Multiple pathways exist for the subsequent storage and utilization of captured carbon dioxide. Sequestration strategies include injection into depleted oil and natural gas reservoirs, mineralization within deep geological rock formations, and utilization of carbon dioxide as a feedstock for the production of value-added products. Regardless of the targeted pathway, a comprehensive understanding of the porous materials engineered to store carbon dioxide under elevated pressures is critical.

In this study, the AccuSorp HP was utilized to evaluate high-pressure carbon dioxide adsorption isotherms across a diverse suite of materials, including molecular sieve 4A, 5A, 13X, and a commercial activated carbon from Supelco. This work establishes a framework for collecting high-pressure carbon dioxide adsorption data utilizing the advanced capabilities of the AccuSorp HP.

Experimental

In this work, CO2 adsorption isotherms were collected on the AccuSorp HP for molecular sieve 4A, 5A, 13X, and Supelco carbon. These isotherms were collected at three temperatures: 15, 25, and 35 ˚C and analyzed up to a maximum pressure of 45 bar. A maximum pressure of 45 bar was chosen for these analyses as the saturation pressure of CO2 is roughly 50 bar at 15 ˚C, the AccuSorp HP can operate up to a maximum pressure of 200 bar for non-condensable fluids. Limiting the maximum pressure ensured that no condensation would occur within the sample tubes. The AccuSorp HP software will prevent users from analyzing gases at pressures up to or above the saturation pressure, removing the requirement for users to search for the saturation pressure of any gas at their chosen analysis temperature.

Prior to analysis, samples were degassed ex-situ using a VacPrep. All tested samples were degassed at 300 ˚C for 8 hours, as they exhibited high thermal stability and structural degradation upon heating was not a concern. The samples were then transferred to the AccuSorp HP for analysis. The sample holder used consisted of a 2 mL stainless steel sample holder.

To maintain the analysis temperature, an iso controller was set to temperatures of 15, 25, or 35 ˚C for the respective analyses. To obtain the appropriate adsorbed quantity, blank corrections were used as CO2 deviates significantly from ideal gas behavior especially at high pressure.

Adsorptive GasCO2
Analysis Temperature298.15K
Free Space TypeMeasure Before
Temperature ControlCirculating Bath
Absolute Tolerance5 mbar
Relative Tolerance5%
Min Pressure Equilibration Time60 s
Max Pressure Equilibration Time99999 s
Pressure Increment (bar)Equilibration Interval (s)Pressure (bar)
0.3601
16010
56040

6045

Table 1: Analysis Conditions for the CO2 Adsorption Analyses

Results and Discussion

Adsorption Isotherms

Carbon dioxide adsorption isotherms were collected on the four materials: molecular sieve 4A, 5A, 13X, and Supelco carbon. The collected isotherm data is shown below in Figures 1-4 for measurements collected at 15, 25, and 35 ˚C.

[Figure 1 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png] Figure 1 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png

Figure 1: Molecular sieve 4A CO2 Adsorption Isotherms Collected on the AccuSorp HP up to 45 bar Pressure

[Figure 2 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png] Figure 2 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png

Figure 2: Molecular sieve 5A CO2 Adsorption Isotherms Collected on the AccuSorp HP up to 45 bar Pressure

[Figure 3 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png] Figure 3 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png

Figure 3: Molecular sieve 13X CO2 Adsorption Isotherms Collected on the AccuSorp HP up to 45 bar Pressure

[Figure 4 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png] Figure 4 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png

Figure 4: Supelco Carbon CO2 Adsorption Isotherms Collected on the AccuSorp HP up to 45 bar Pressure

Across all samples, the expected trend of decreasing adsorption capacity with increasing temperature was observed. For the three samples, strong adsorption was present at low temperatures as expected of highly microporous samples. The Supelco carbon showed lower CO2 adsorption at low pressure, but excellent capacity once higher pressures were achieved. When comparing the samples at 1 bar of pressure, the 13X displays the strongest CO2 adsorption followed by molecular sieve 5A, then 4A, and lastly Supelco carbon. At a pressure of 45 bar, molecular sieve 13X maintains the highest capacity, followed closely by Supelco carbon, then molecular sieve 5A, and lastly 4A.

The takeaway from these isotherm measurements is that low pressure adsorption is primarily dominated by adsorption of CO2 within the smallest pores of the material. At high pressure, the maximum adsorption is primarily driven by the total pore volume of the material. Molecular sieves 4A and 5A have very small pores that facilitate strong adsorption at low pressure but lack the total volume when compared to 13X and Supelco carbon. For this reason, these materials completely fill the pore volume quickly and at relatively low pressures.

Heat of Adsorption Reporting

The collected isothermal data from the AccuSorp HP integrates with the MicroActive software suite, enabling heat of adsorption reporting. This allows users to evaluate heat of adsorption of their materials across the range of adsorption coverages. Heat of adsorption is the amount of energy that is released upon adsorption of the adsorbing molecule onto the surface of a material. Higher numbers indicate a stronger interaction. Figure 5 below shows the calculated heats of adsorption for the four materials analyzed in this study.

[Figure 5 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png] Figure 5 AN260630-co2-adsorption-data-accusorp-zeolite-carbon.png

Figure 5: CO2 Heat of adsorption plots for 4A (top left), 5A (top right), 13X (bottom left), and Supelco carbon (bottom right)

The results from the heat of adsorption report are consistent with earlier observations from the isothermal data that was obtained on the molecular sieve and carbon materials. The three materials display large heats of adsorption, nearly 50 kJ/mol at zero coverage, which decreases at increasing coverage. The loss in heat of adsorption energy with decreasing coverage is most pronounced for the molecular sieve 4A and 5A materials. In comparison, the Supelco carbon exhibits a significantly lower heat of adsorption compared to the molecular sieve materials at zero coverage; however, it remained stable with increasing coverage, maintaining a value near 25 kJ/mol.

Conclusion

This application note provides an overview of high-pressure carbon dioxide adsorption characterization using the AccuSorp HP. Comparative adsorption evaluations were conducted across molecular sieve 4A, 5A, 13X, and a commercial Supelco activated carbon. These exhibited strong affinity for carbon dioxide adsorption, as was evident from their high isosteric heats of adsorption within the range of 45 to 50 kJ/mol at low surface coverage. The Supelco carbon and molecular sieve 13X both displayed excellent high-pressure adsorption of carbon dioxide, reaching capacities near 7 mmol/g at the maximum evaluated pressure of 45 bar.